| INJECTION MOULDING | ||||
|
MATERIALS |
BARREL TEMPERATURE (oC) |
MOULD TEMPERATURE (oC) |
INJECTION PRESSURE (PSI) |
MOULD SHRINKAGE (%) |
|
Low Density Polyethylene |
145-260 |
10-60 |
18800 |
1.5-3.5 |
|
High Density Polyethylene |
160-270 |
5-50 |
26000 |
1.5-3.0 |
|
Poly Propylene |
190-210 |
5-80 |
26100 |
1.0-3.0 |
|
Poly Styrene |
180-280 |
10-80 |
21400 |
0.2-0.8 |
|
High Impact Polystyrene |
170-270 |
10-80 |
21400 |
0.3-0.6 |
|
Styrene Acrylonitrile |
180-270 |
30-85 |
21400 |
0.2-0.6 |
|
Acrylonitrile – Butodiene Styrene |
180-240 |
60-90 |
21400 |
0.5-0.7 |
|
Polymethyl Methacrylate |
180-260 |
40-80 |
25000 |
0.2-0.4 |
|
Unplasticised Polyrinyl Chloride |
170-210 |
20-60 |
25000 |
0.2-0.4 |
|
Plasticised Polyvinyl Chloride |
160-185 |
20-30 |
17400 |
1.5-3.0 |
|
Poly Vinylidene Fluoride |
180-250 |
30-120 |
21400 |
3.0 |
|
Cellulose Acetate |
170-250 |
40-80 |
21400 |
0.2-0.5 |
|
Cellulose Acetate Butyrate |
170-230 |
40-80 |
21400 |
0.2-0.5 |
|
Cellulose Propionoate |
170-250 |
40-80 |
21400 |
0.2-0.5 |
|
Poly Carbonate |
280-320 |
85-120 |
29000 |
0.5-0.7 |
|
Poly Ether Sulphone |
320-420 |
130-200 |
29000 |
0.8 |
|
Poly Phenylene-Oxide (Modified) |
230-275 |
80-110 |
21400 |
0.7-0.8 |
|
Poly Oxymethylene (Acetal) |
180-220 |
40-120 |
10700 |
0.2-0.7 |
|
Poly Phenylene Sulphide |
310-330 |
130-160 |
21800 |
0.7-0.8 |
|
Poly Butylene Terephthalate |
260-280 |
70-140 |
29000 |
0.9-1.2 |
|
Poly Ethylene Terephthalate |
230-260 |
60-120 |
29000 |
0.9-1.2 |
|
Nylon 6 |
230-260 |
60-90 |
21400 |
0.7-1.5 |
|
Nylon 6.6 |
260-290 |
60-100 |
21400 |
1.0-2.5 |
|
Nylon 11 |
210-250 |
60-80 |
21400 |
1.0-2.5 |
|
Nylon 12 |
210-250 |
60-80 |
21400 |
0.8-2.0 |
|
Thermoplastic Polyurethane |
170-220 |
15-65 |
17200 |
1.0 |
|
Thermoplastic Polyetherester |
160-180 |
10-70 |
18000 |
0.4-1.6 |
|
Rubber Reinforced PP |
210-270 |
20-60 |
26100 |
0.2 |
|
SBS Block/ Copolymers |
150-200 |
15-65 |
11600 |
1.0 |
|
Structural Form |
150-220 |
10-60 |
21400 |
2.0 |